Molybdenum Disulfide (MoS2) Application Process:
- Cleaning: Parts are cleaned to remove all oil, grease & other substances. Cast parts are de-gassed.
- Pretreatment: Abrasive blast surface with 180-220 grit aluminum oxide Phosphate IAW MIL-DTL-16232, type M, class 3 or type Z, class 3
- Material Preperation: MoS2 is rolled at 30 rpm for 30 minutes to ensure the coating has been adequately mixed.
- Application: The coating is sprayed onto the item either manually or on one our automated production lines.
- Cure / Bake: Depending on the coating used the part is cured in an oven at a temperature from 300°F to 400°F.
- Inspection: Parts are inspected to ensure proper application.